WO2023039668A1 - Procédés de récupération de vanadium sous la forme d'un électrolyte au vanadium et utilisations associées - Google Patents
Procédés de récupération de vanadium sous la forme d'un électrolyte au vanadium et utilisations associées Download PDFInfo
- Publication number
- WO2023039668A1 WO2023039668A1 PCT/CA2022/051371 CA2022051371W WO2023039668A1 WO 2023039668 A1 WO2023039668 A1 WO 2023039668A1 CA 2022051371 W CA2022051371 W CA 2022051371W WO 2023039668 A1 WO2023039668 A1 WO 2023039668A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- vanadium
- molar
- vanadyl sulfate
- extractant
- leaching
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
La présente demande concerne un procédé de récupération de vanadium sous la forme d'une solution de sulfate de vanadyle à partir d'une source secondaire de vanadium par un procédé de lixiviation réductrice utilisant un saccharide et de l'acide sulfurique. La source secondaire de vanadium comprend des cendres volantes d'huile, du coke de pétrole, des résidus de pétrole riches en vanadium, du laitier de vanadium et des catalyseurs au vanadium usés. La solution de sulfate de vanadyle peut être utilisée en tant qu'électrolyte au vanadium dans une batterie à flux redox au vanadium.
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CA3232000A CA3232000A1 (fr) | 2021-09-15 | 2022-09-14 | Procedes de recuperation de vanadium sous la forme d'un electrolyte au vanadium et utilisations associees |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US202163261219P | 2021-09-15 | 2021-09-15 | |
| US63/261,219 | 2021-09-15 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023039668A1 true WO2023039668A1 (fr) | 2023-03-23 |
Family
ID=85601856
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/CA2022/051371 Ceased WO2023039668A1 (fr) | 2021-09-15 | 2022-09-14 | Procédés de récupération de vanadium sous la forme d'un électrolyte au vanadium et utilisations associées |
Country Status (2)
| Country | Link |
|---|---|
| CA (1) | CA3232000A1 (fr) |
| WO (1) | WO2023039668A1 (fr) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN119080063A (zh) * | 2024-08-30 | 2024-12-06 | 广东省科学院资源利用与稀土开发研究所 | 一种钒渣钙化焙烧酸浸液萃取法短流程制备高纯硫酸氧钒的新方法及其产品 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4721606A (en) * | 1982-08-20 | 1988-01-26 | Union Oil Company Of California | Recovery of metal values from spent catalysts |
| WO2004099079A1 (fr) * | 2003-05-12 | 2004-11-18 | Clean Teq Pty Ltd | Procede de production de solution electrolytique contenant du vanadium |
| CN101289705A (zh) * | 2007-04-20 | 2008-10-22 | 北京化工大学 | 一种从钒铁矿炼铁废渣中提取钒的方法 |
| US20180209014A1 (en) * | 2015-07-15 | 2018-07-26 | National University Corporation Gunma University | Vanadium Recovery Method, Method for Producing Electrolytic Solution for Redox Flow Batteries, Vanadium Recovery Device, and Device for Producing Electrolytic Solution for Redox Flow Batteries |
| JP2018168012A (ja) * | 2017-03-29 | 2018-11-01 | ブラザー工業株式会社 | 硫酸バナジウム(iii )の製造方法、電極前駆体の製造方法、及びバナジウムレドックス二次電池の製造方法 |
-
2022
- 2022-09-14 WO PCT/CA2022/051371 patent/WO2023039668A1/fr not_active Ceased
- 2022-09-14 CA CA3232000A patent/CA3232000A1/fr active Pending
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4721606A (en) * | 1982-08-20 | 1988-01-26 | Union Oil Company Of California | Recovery of metal values from spent catalysts |
| WO2004099079A1 (fr) * | 2003-05-12 | 2004-11-18 | Clean Teq Pty Ltd | Procede de production de solution electrolytique contenant du vanadium |
| CN101289705A (zh) * | 2007-04-20 | 2008-10-22 | 北京化工大学 | 一种从钒铁矿炼铁废渣中提取钒的方法 |
| US20180209014A1 (en) * | 2015-07-15 | 2018-07-26 | National University Corporation Gunma University | Vanadium Recovery Method, Method for Producing Electrolytic Solution for Redox Flow Batteries, Vanadium Recovery Device, and Device for Producing Electrolytic Solution for Redox Flow Batteries |
| JP2018168012A (ja) * | 2017-03-29 | 2018-11-01 | ブラザー工業株式会社 | 硫酸バナジウム(iii )の製造方法、電極前駆体の製造方法、及びバナジウムレドックス二次電池の製造方法 |
Non-Patent Citations (1)
| Title |
|---|
| KOVALEV ANATOLY, WAINSTEIN DMITRY, VAKHRUSHEV VLADIMIR, VOLKOV ANTON, KOLOGRIEVA ULYANA: "Features of the Microstructure and Chemical Compositions of Vanadium-Containing Slags Including Determination of Vanadium Oxidation Degrees", MATERIALS, vol. 12, no. 21, pages 3578, XP093049465, DOI: 10.3390/ma12213578 * |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN119080063A (zh) * | 2024-08-30 | 2024-12-06 | 广东省科学院资源利用与稀土开发研究所 | 一种钒渣钙化焙烧酸浸液萃取法短流程制备高纯硫酸氧钒的新方法及其产品 |
Also Published As
| Publication number | Publication date |
|---|---|
| CA3232000A1 (fr) | 2023-03-23 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US20230115288A1 (en) | Processing for the extraction of rare earth elements | |
| Li et al. | Extraction of vanadium from black shale using pressure acid leaching | |
| JP5881603B2 (ja) | 水溶液から金属を回収する方法 | |
| CN102191391B (zh) | 从高杂质低品位的复杂氧化锌粉中提取锗的方法 | |
| AU2013238535B2 (en) | Method for producing high-purity nickel sulfate | |
| Cai et al. | Comprehensive recovery of metals in spent Ni–Mo/γ–Al2O3 hydrofining catalyst | |
| Hu et al. | Separation and recovery of iron impurity from a vanadium-bearing stone coal via an oxalic acid leaching-reduction precipitation process | |
| CN104831075A (zh) | 一种废钒钼系scr催化剂的钒、钼分离和提纯方法 | |
| CN101967563A (zh) | 一种利用含钒钛转炉渣的湿法提钒方法 | |
| WO2010111548A2 (fr) | Procédé de récupération de métaux de catalyseurs épuisés contenant des résidus de liquéfaction du charbon | |
| US11807544B2 (en) | Selective recovery method of vanadium and cesium from waste sulfuric acid vanadium catalyst, and high-quality vanadium aqueous solution and cesium alum produced thereby | |
| Chang et al. | Recovery of vanadium from black shale | |
| CN1900330A (zh) | 一种低污染沉矾除铁湿法炼锌方法 | |
| Habinshuti et al. | Caustic potash assisted roasting of the Nigerian ferro-columbite concentrate and guanidine carbonate-induced precipitation: a novel technique for extraction of Nb–Ta mixed-oxides | |
| WO2023039668A1 (fr) | Procédés de récupération de vanadium sous la forme d'un électrolyte au vanadium et utilisations associées | |
| CN1861817A (zh) | 从磁铁矿尾渣中提取金属钴的工艺 | |
| Kurniawan et al. | Intensified extraction of vanadium from vanadium-bearing titanomagnetite (VTM) concentrate via one-stage leaching and solvent extraction using acidic organophosphorus extractant | |
| CN113149075A (zh) | 一种从低品位铌矿中制备五氧化二铌的方法 | |
| Zhang et al. | Enhancing the leaching performance of molybdenite and Co-white alloy simultaneously: A structure conversion process | |
| CN113735179B (zh) | 一种利用铁锰制备高纯硫酸铁的方法 | |
| CN118792526A (zh) | 一种从尾矿中提取富铌浸出液的方法 | |
| CN104975192A (zh) | 从含钪物料中提取钪的方法 | |
| Zhang et al. | Recovery of vanadium from Ba3 (VO4) 2 precipitate obtained from processing of Bayer vanadium sludge: NaHCO3 leaching behaviors and V2O5 preparation | |
| Pandey | Rare metals extraction from non-ferrous resources in India: Present status and prospects of R&D | |
| KR101222588B1 (ko) | 휘수연석으로부터 몰리브덴의 선택적 침전방법 및 그 방법을 이용한 레늄 분리방법 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22868496 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 3232000 Country of ref document: CA |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 22868496 Country of ref document: EP Kind code of ref document: A1 |