WO2004110724A1 - 二層構造ブッシュの成形金型 - Google Patents
二層構造ブッシュの成形金型 Download PDFInfo
- Publication number
- WO2004110724A1 WO2004110724A1 PCT/JP2003/007520 JP0307520W WO2004110724A1 WO 2004110724 A1 WO2004110724 A1 WO 2004110724A1 JP 0307520 W JP0307520 W JP 0307520W WO 2004110724 A1 WO2004110724 A1 WO 2004110724A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- mold
- rubber
- molding
- die
- stage
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
Description
Claims