US20010042575A1 - Apparatus and method for suppressing growth of oxide film on coil - Google Patents
Apparatus and method for suppressing growth of oxide film on coil Download PDFInfo
- Publication number
- US20010042575A1 US20010042575A1 US09/918,546 US91854601A US2001042575A1 US 20010042575 A1 US20010042575 A1 US 20010042575A1 US 91854601 A US91854601 A US 91854601A US 2001042575 A1 US2001042575 A1 US 2001042575A1
- Authority
- US
- United States
- Prior art keywords
- coil
- oxide film
- covers
- suppressing growth
- cooling
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Abandoned
Abstract
An apparatus and a method for suppressing growth of an oxide film on a coil which is a spirally wound, rolled strip are disclosed. A rolled strip subjected to rolling by hot rolling equipment is wound spirally by a down-coiler to make a coil. Covers are disposed on the opposite sides of the coil such that heat resistant materials intimately contact the opposite sides of the coil. The covers are fixed by L-bolts and nuts to cover the opposite sides of the coil with the covers. In this state, the coil is naturally cooled for a predetermined time to suppress growth of an oxide film and increase productivity.
Description
- 1. Field of the Invention
- The present invention relates to an apparatus and a method for suppressing growth of an oxide film on a coil of a rolled strip which has been wound from hot rolling equipment onto a down-coiler and stored in a coil yard.
- 2. Description of the Related Art
- FIGS. 13(a) and 13(b) schematically show a general state of storage of the coils. FIG. 14 is a graph showing the thickness of an oxide film, in the width direction, on the coil in a conventional state of storage.
- A rolled strip after rolling in hot rolling equipment is wound spirally by a down-coiler, carried to a coil yard, and stored there. The posture of the coil in storage is a horizontal posture of a coil C as shown in FIG. 13( a), or a vertical posture of the coil C as shown in FIG. 13(b). In this posture of storage, the coils are placed in a layer, or stacked in layers, on a frame (not shown) . The coils stored in that posture are cooled by natural ventilation or forced cooling in a building for about 110 hours in summer, or about 80 hours in winter.
- In the above posture of coil storage, the rolled strip is cooled in the coil yard while being left to stand for a long time at a high temperature in an oxidizing atmosphere of the air. Thus, an oxide film grows on the surface of the coil over a long time. In the case of the coil of the rolled strip spirally wound, both of its edges directly touch the air. From the edges, air penetrates the gap between the adjacent turns of the rolled strip. Consequently, the oxide film growing on the strip surface of the coil differs in thickness in its width direction.
- The graph indicated in FIG. 14 shows the thickness of the oxide film in the width direction of the coil. During rolling, the oxide film is formed uniformly to a thickness of 8 μm, and then the coil is cooled for a predetermined period of time in the coil yard. As shown in this graph, the oxide film on the strip surface of the coil grows to a thickness of 18 μm at the edge, 15 μm at a distance of 50 mm from the edge, 9 μm at a distance of 300 mm from the edge, and 8.5 μm at a distance of 470 mm from the edge (i.e., at a central position in the width direction). One will see that when the rolled strip in the coiled form is cooled, the oxide film grows to a thickness of 8.5 μm at the central position in the width direction, but to a thickness of 18 μm, a value more than two-fold, at the edge.
- The rolled strip having the oxide film formed on the surface thereof is generally acid pickled to remove the oxide film. Then, the rolled strip is transported to a subsequent step such as a plating line. The acid pickling of the rolled strip is performed by guiding the rolled strip into an acid pickling tank holding an acid liquid, and immersing the rolled strip therein for a predetermined time, thereby cleaning off the oxide film formed on the surface. That is, the duration of immersion of the rolled strip in the acid pickling tank is set in accordance with the thickness of the oxide film formed on the surface of the rolled strip. Hence, the rolled strip, which has the oxide film 8.5 μm thick at the central position and 18 μm at the edge, needs to be immersed in the acid pickling tank for a long time adapted for the
oxide film 18 μm in thickness. As a result, the transport speed of the rolled strip in acid pickling is slowed, decreasing the overall production efficiency. When the thickness of the oxide film formed on the surface of the rolled strip is great, moreover, the consumption of the acid liquid used increases, raising the pickling cost. - The present invention has been accomplished to solve the above-described problems with the earlier technologies. It is an object of this invention to provide an apparatus and a method for suppressing growth of an oxide film on a coil of a rolled strip by properly storing and cooling the coil, while achieving an increase in productivity.
- An aspect of the invention, as a means of attaining the above object, is an apparatus for suppressing growth of an oxide film on a coil which is a spirally wound, rolled strip, wherein covers are provided for covering at least opposite sides of the coil.
- Thus, the opposite sides of the coil are cooled while being shielded from the outside air. Penetration of air into the interior of the coil is inhibited, the growth of the oxide film on the rolled strip (coil), especially at its edge, is suppressed, and the formation of an oxide film extremely thick at the edge compared with the center in the width direction can be prevented. As a result, the coil has an oxide film overall thin, and widthwise leveled in thickness. The acid pickling time for cleaning off the oxide film can be markedly decreased, and the transport speed of the rolled strip during acid pickling can be increased, whereby the overall production efficiency can be raised. The consumption of the acid liquid used can also be decreased to reduce the pickling cost.
- In the apparatus for suppressing growth of an oxide film on a coil, a heat insulating material may be provided on a surface of each of the covers in intimate contact with the coil. By this measure, rapid local cooling of the coil is prevented, and penetration of air into the interior of the coil is reliably inhibited. Consequently, the formation of an oxide film extremely thick at the edge compared with the center in the width direction can be prevented. The resulting oxide film is overall thin, and widthwise leveled in thickness.
- In the apparatus for suppressing growth of an oxide film on a coil, each of the covers may be shaped like a ring having a through-hole at a center thereof, and eye rings formed to project toward the through-holes of the covers may be connected together and fixed by bolts and nuts. By these measures, the covers can be mounted easily on the coil.
- In the apparatus for suppressing growth of an oxide film on a coil, a cooling water path may be provided in each of the covers. By this measure, the coil is forcedly cooled with cooling water, with its opposite sides being shielded from the outside air. Consequently, the cooling time can be shortened, and the storage time of the coil in the coil yard can be reduced.
- In the apparatus for suppressing growth of an oxide film on a coil, each of the covers may be shaped like a disk having a flange portion in an outer peripheral area of the cover, and the cooling water path may be provided along a circumferential direction of the cover. Since the cooling water path becomes long, the cooling efficiency can be increased.
- In the apparatus for suppressing growth of an oxide film on a coil, the covers may be provided with a supply path and a discharge path for supplying and discharging an inert gas into and from a hollow portion of the coil. By this measure, the opposite sides of the coil are shielded from the outside air, and the hollow portion of the coil is supplied with the inert gas. Thus, penetration of air into the interior of the coil is inhibited, and the oxidizing atmosphere inside the coil is purged with the inert gas. Consequently, growth of the oxide film on the rolled strip can be suppressed reliably.
- In the apparatus for suppressing growth of an oxide film on a coil, each of the covers may be shaped like a disk having a flange portion in an outer peripheral area of the cover, and the supply path and the discharge path for the inert gas which communicate with the hollow portion of the coil may be provided in the center of the covers. By this measure, a simple constitution can increase the cooling efficiency.
- In the apparatus for suppressing growth of an oxide film on a coil, the covers may be a cup for accommodating the coil and a cap for covering an opening of the cup. By so doing, the coil can be cooled, with its whole being shielded from the outside, so that the growth of the oxide film on the rolled strip can be suppressed reliably.
- Another aspect of the invention is a method for suppressing growth of an oxide film on a coil which is a spirally wound, rolled strip, comprising cooling the coil while covering at least opposite sides of the coil with covers.
- Thus, penetration of air into the interior of the coil can be inhibited, the growth of the oxide film on the rolled strip (coil), especially at its edge, can be suppressed, and the formation of an oxide film extremely thick at the edge compared with the center in the width direction can be prevented. As a result, the coil has an oxide film overall thin, and widthwise leveled in thickness.
- The method for suppressing growth of an oxide film on a coil may comprise cooling the coil while heat insulating surfaces of the covers and the coil in intimate contact with each other. By so doing, rapid local cooling of the coil is prevented, and penetration of air into the interior of the coil is reliably inhibited. Consequently, the formation of an oxide film extremely thick at the edge compared with the center in the width direction can be prevented. The resulting oxide film becomes overall thin and widthwise leveled in thickness.
- The method for suppressing growth of an oxide film on a coil may comprise cooling the coil by flowing cooling water in a cooling water path provided in each of the covers. By so doing, the coil is forcedly cooled with cooling water, with its opposite sides being shielded from the outside air. Consequently, the cooling time can be shortened, and the storage time of the coil in the coil yard can be reduced.
- The method for suppressing growth of an oxide film on a coil may comprise cooling the coil while supplying and discharging an inert gas into and from a hollow portion of the coil. By so doing, the opposite sides of the coil are shielded from the outside air, and the hollow portion of the coil is supplied with the inert gas. Thus, penetration of air into the interior of the coil can be inhibited, and the oxidizing atmosphere inside the coil can be purged with the inert gas. Consequently, growth of the oxide film on the rolled strip can be suppressed reliably.
- The method for suppressing growth of an oxide film on a coil may comprise cooling the coil in an accommodated state. By so dong, the coil can be cooled, with its whole being shielded from the outside, so that the growth of the oxide film on the rolled strip can be suppressed reliably.
- The above and other objects, features and advantages of the present invention will become more apparent from the following description taken in connection with the accompanying drawings, in which:
- FIG. 1 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a first embodiment of the present invention, designed to carry out a method for suppressing growth of an oxide film on a coil;
- FIG. 2 is a side view of the apparatus for suppressing growth of an oxide film on a coil;
- FIG. 3 is an exploded perspective view of the apparatus for suppressing growth of an oxide film on a coil;
- FIG. 4 is a graph showing the thickness of an oxide film in a width direction of a coil in the apparatus for suppressing growth of the oxide film on the coil according to the first embodiment;
- FIG. 5 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a second embodiment of the invention;
- FIG. 6 is a side view of the apparatus for suppressing growth of an oxide film on a coil;
- FIG. 7 is a graph showing the thickness of an oxide film in a width direction of a coil in the apparatus for suppressing growth of the oxide film on the coil according to the second embodiment;
- FIG. 8 is a graph showing the temperature of the coil versus the cooling time for the coil;
- FIG. 9 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a third embodiment of the invention;
- FIG. 10 is a side view of the apparatus for suppressing growth of an oxide film on a coil;
- FIG. 11 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a fourth embodiment of the invention;
- FIG. 12 is a side view of the apparatus for suppressing growth of an oxide film on a coil;
- FIGS. 13(a) and 13(b) are each a schematic view showing a general storage state of the coils; and
- FIG. 14 is a graph showing the thickness of an oxide film in a width direction of a coil in a conventional storage state.
- Embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which in no way limit the invention.
- [First Embodiment]
- FIG. 1 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a first embodiment of the invention, designed to carry out a method for suppressing growth of an oxide film on a coil. FIG. 2 is a side view of the apparatus for suppressing growth of an oxide film on a coil. FIG. 3 is an exploded perspective view of the apparatus for suppressing growth of an oxide film on a coil. FIG. 4 is a graph showing the thickness of an oxide film in a width direction of a coil in the apparatus for suppressing growth of the oxide film on the coil according to the present embodiment.
- As shown in FIGS. 1 to 3, a coil C is rolled by hot rolling equipment (not shown), and then spirally wound by a down-coiler. The resulting coil is transported to a coil yard, where it is stored by an
apparatus 10 for suppressing growth of an oxide film on a coil according to the present embodiment. Thisapparatus 10 is composed of a pair of covers (right and left covers) 11, 12 for covering opposite sides of the coil C, and two L-bolts 13 and twonuts 14 as connectors for fixing thecovers 11, 12 to the opposite sides of the coil C. The covers 11, 12 are of the same structure, and have nearly the same diameter as (or a slightly larger diameter than) the diameter of the coil C. The covers 11 and 12 are shaped like rings having through- 15 and 16, respectively, in the center. On the inner peripheral surface of the through-holes 15 and 16, two eye rings 17 and two eye rings 18 are fixed. To a surface of each of theholes covers 11 and 12, heat 19 and 20 having elasticity and heat insulating properties are attached which have a ring shape to be brought into intimate contact with the respective edges of the coil C. Theresistant materials reference numeral 21 denotes a coil storing frame for bearing the coil C. - A rolled strip subjected to rolling by the hot rolling equipment is wound spirally by the down-coiler to make a coil C. The coil C is transported to the coil yard, and borne on the
coil storing frame 21. On thecoil storing frame 21, thecovers 11, 12 are disposed on the opposite sides of the coil C such that the heat 19, 20 intimately contact the opposite sides of the coil C. The L-resistant materials bolts 13 are passed through the eye rings 17 of one cover 11, a hollow hole of the coil C, and the eye rings 18 of theother cover 12, whereafter the nuts 14 are screwed on front end portions of the L-bolts 13. In this manner, thecovers 11, 12 are mounted on the coil C so as to cover its opposite sides. - When the
covers 11, 12 have been mounted on the opposite sides of the coil C via the heat 19, 20, the coil C is naturally cooled in this condition for a predetermined period of time in the coil yard. During this cooling treatment, theresistant materials covers 11, 12 are mounted on the opposite sides of the coil C via the heat 19, 20 to close open ends of a gap between the adjacent spiral turns of the rolled strip in the coil C, thereby inhibiting penetration of air into the interior of the coil C. Thus, growth of an oxide film on the rolled strip (coil C), especially at its edge, is suppressed, and the formation of an oxide film extremely thick at the edge compared with the center in the width direction can be prevented.resistant materials - The graph as FIG. 4 shows the thickness of the oxide film in the width direction of the coil C which has been cooled for a predetermined time in the coil yard after the oxide film was formed uniformly to a thickness of 8 μm during rolling. As shown in this graph, the thickness of the oxide film growing on the strip surface of the coil is 9.5 μm at the edge, and 8.5 μm at a distance of 470 mm from the edge (i.e., at the central position in the width direction). There is substantially no difference between the two thicknesses, indicating that the thickness of the oxide film is almost leveled in the width direction.
- The above finding points to the prevention of the phenomenon that the oxide film becomes extremely thick only at the edge during cooling of the coil C after rolling. The overall thickness of the oxide film becomes small. The acid pickling time for cleaning off the oxide film can be markedly decreased, and the transport speed of the rolled strip during acid pickling can be increased, whereby the overall production efficiency can be raised. The consumption of the acid liquid used can also be decreased to reduce the pickling cost. Furthermore, wasteful removal of the material other than the oxide film, namely, the base material, is decreased, and the quality of the product can be improved.
- [Second Embodiment]
- FIG. 5 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a second embodiment of the invention. FIG. 6 is a side view of the apparatus for suppressing growth of an oxide film on a coil. FIG. 7 is a graph showing the thickness of an oxide film in a width direction of a coil in the apparatus for suppressing growth of the oxide film on the coil according to the present embodiment. FIG. 8 is a graph showing the temperature of the coil versus the cooling time for the coil. Members having the same functions as illustrated in the above-mentioned embodiment are assigned the same reference numerals, and their explanations will be omitted.
- As shown in FIGS. 5 and 6, an
apparatus 30 for suppressing growth of an oxide film on a coil has a pair of covers (right and left covers) 31 and 32 fitted on a coil C so as to cover its opposite sides. In each of the 31 and 32, a cooling water path is provided, and a supply path and a discharge path are provided for supplying and discharging an inert gas into and from a hollow portion of the coil C. The covers 31, 32 are of the same structure, and have a slightly larger diameter than the diameter of the coil C. The covers 31 and 32 are shaped like disks havingcovers 33 and 34 in the outer peripheral area of the cover, theflange portions 33 and 34 being fitted around the outer periphery at each end of the coil C. In theflange portions 31 and 32, coolingcovers 35 and 36 are formed as the cooling water paths. One end of each of the coolingwater channels 35, 36 is connected to a cooling water source (not shown) via coolingwater channels 37, 38 joined to upper parts of thewater supply pipes 31, 32. The other end of each of the coolingcovers 35, 36 is coupled to coolingwater channels 39, 40 joined to lower parts of thewater discharge pipes 31, 32. Cooling water from cooling equipment may be forcedly passed through the coolingcovers 35, 36 by a pump, and after cooling, may be circulated to the cooling equipment. To one of the covers, 31, awater channels gas supply pipe 41 for supplying an inert gas into the hollow portion of the coil C is connected via a pipe joint 42. To the other cover, 32, agas discharge pipe 43 for discharging the inert gas, which has been supplied into the hollow portion of the coil C, is connected via a pipe joint 44. As the inert gas, an N2 gas or an Ar gas is preferred in order to purge an oxidizing atmosphere. Such an inert gas may be forced into the hollow portion of the coil C at room temperature by a pump. - The coil C borne on a
coil storing frame 21 is mounted by having its opposite sides fitted with the 33 and 34 of theflange portions 31 and 32. By forcibly flowing cooling water from the cooling equipment into the coolingcovers 35 and 36 via the coolingwater channels 37 and 38 by means of the pump, the coil C is indirectly cooled. Also, by forcibly flowing the inert gas from thewater supply pipes gas supply pipe 41 into the hollow portion of the coil C via the pipe joint 42 by means of the pump, the coil C is cooled, and the oxidizing atmosphere is purged. In this manner, the coil C is forcedly cooled for a predetermined time in the coil yard. - During this cooling treatment, the
31 and 32 are attached to the opposite sides of the coil C to close the open ends of the gap between the spiral turns of the rolled strip in the coil C. Thus, penetration of air into the interior of the coil C is inhibited. At the same time, the inert gas is supplied into the hollow portion of the coil C to purge the inside oxidizing atmosphere. Hence, growth of an oxide film on the rolled strip (coil C) is suppressed, and the formation of an oxide film extremely thick at the edge compared with the center in the width direction is prevented. That is, as shown in FIG. 7, the thickness of the oxide film growing on the strip surface of the coil C is smaller than 9 μm at the central position in the width direction, as well as at the edge, indicating that the thickness of the oxide film is almost leveled in the width direction.covers - The graph as FIG. 8 shows the temperature of the coil versus the cooling time for the coil, making a comparison between natural cooling of the coil C allowed to stand in the coil yard, and forced cooling of the coil C performed by flowing cooling water in the
31 and 32 and flowing the inert gas into the hollow portion of the coil C. As this graph shows, the cooling time to a predetermined temperature is shortened by about 20% in the forced cooling in comparison with the natural cooling.covers - The above findings point to the prevention of the phenomenon that the oxide film becomes extremely thick only at the edge during cooling of the coil C after rolling. The overall thickness of the oxide film becomes small. The acid pickling time for cleaning off the oxide film can be markedly decreased, and the transport speed of the rolled strip during acid pickling can be increased, whereby the overall production efficiency can be raised. The consumption of the acid liquid used can also be decreased to reduce the pickling cost. Furthermore, wasteful removal of the material other than the oxide film, namely, the base material, is decreased, and the quality of the product can be improved. Besides, the coil C is forcedly cooled to shorten the cooling time. Thus, the storage time of the coil C in the coil yard can be reduced.
- In the present embodiment, the
31, 32 have been mounted by fitting thecovers 33, 34 onto the opposite sides of the coil C. However, joints may be formed on the outer periphery of theflange portions 31, 32, and L-bolts and nuts may be used supplementally to fix thecovers 31, 32, as in the aforementioned embodiment.covers - [Third Embodiment]
- FIG. 9 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a third embodiment of the invention. FIG. 10 is a side view of the apparatus for suppressing growth of an oxide film on a coil.
- As shown in FIGS. 9 and 10, an
apparatus 50 for suppressing growth of an oxide film on a coil is composed of a cup (cover) 51 for accommodating a coil C so as to cover a side portion of the coil C, and acap 52 fitted on thecup 51 so as to cover the other side portion of the coil C. Thecup 51 is made of steel, takes a cylindrical shape, and has an inner peripheral portion slightly larger in diameter than the coil C. Thecap 52 is also made of steel, takes a cylindrical shape, and has an inner peripheral portion which can be fitted around an outer peripheral portion of thecup 51. The coil C is fitted with thecup 51 while being supported by an L-shaped fork. Then, the coil C is borne on acoil storing frame 21, and thecap 52 is fitted on thecup 51 to accommodate the coil C. When the coil C has been accommodated in thecup 51 and thecap 52 in this manner, the coil C is naturally cooled for a predetermined time in this state in the coil yard. During the cooling treatment, therefore, the coil C is shielded from the outside air, so that the growth of an oxide film on the rolled strip (coil C) is suppressed. This results in the prevention of the phenomenon that the oxide film becomes extremely thick only at the edge during cooling of the coil C after rolling. The overall thickness of the oxide film becomes small. Furthermore, the coil C is accommodated in thecup 51 and thecap 52 and naturally cooled over a long time. Hence, the ductility of the rolled strip (steel plate) can be improved because of an annealing effect. - [Fourth Embodiment]
- FIG. 11 is a partially cutaway front view of an apparatus for suppressing growth of an oxide film on a coil according to a fourth embodiment of the invention. FIG. 12 is a side view of the apparatus for suppressing growth of an oxide film on a coil.
- As shown in FIGS. 11 and 12, an
apparatus 60 for suppressing growth of an oxide film on a coil is composed of a cup (cover) 61 for accommodating a coil C so as to cover a side portion of the coil C, and acap 62 fitted on thecup 61 so as to cover the other side portion of the coil C. Thecup 61 is made of steel, takes a cylindrical shape, and has a laminated structure in which aheat insulating material 63 is mounted on an inner peripheral portion of thecup 61. Thecap 62 is also made of steel, takes a cylindrical shape, and has a laminated structure in which aheat insulating material 64 is mounted on an inner peripheral portion of thecap 62. The coil C is fitted with thecup 61 while being supported by an L-shaped fork. Then, the coil C is borne on acoil storing frame 21, and thecap 62 is fitted on thecup 61 to accommodate the coil C. When the coil C has been accommodated in thecup 61 and thecap 62 in this manner, the coil C is naturally cooled in this state for a predetermined time in the coil yard. During the cooling treatment, therefore, the coil C is shielded from the outside air, so that the growth of an oxide film on the rolled strip (coil C) is suppressed. This results in the prevention of the phenomenon that the oxide film becomes extremely thick only at the edge during cooling of the coil C after rolling. The overall thickness of the oxide film becomes small. Furthermore, the coil C is accommodated in thecup 61 and thecap 62, and shielded from the outside by the 63, 64. In this condition, the coil C is naturally cooled over a long time. Hence, the ductility of the rolled strip (steel plate) can be improved because of an annealing effect.heat insulating materials - In the foregoing respective embodiments, the cover has been formed in many shapes. However, the cover may be any one which can cover the opposite sides of the coil, and is not restricted to these shapes. Furthermore, bolts and nuts, and flange fitting have been used as fixing tools for fixing the cover to the coil, but they are not limitative of the invention.
- The invention being thus described, it will be obvious that the same may be varied in many ways. Such variations are not to be regarded as a departure from the spirit and scope of the invention, and all such modifications as would be obvious to one skilled in the art are intended to be included within the scope of the following claims.
Claims (13)
1. An apparatus for suppressing growth of an oxide film on a coil which is a spirally wound, rolled strip, wherein:
covers are provided for covering at least opposite sides of the coil.
2. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 1
a heat insulating material is provided on a surface of each of the covers in intimate contact with the coil.
3. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 1
each of the covers is shaped like a ring having a through-hole at a center thereof, and eye rings formed to project toward the through-holes of the covers are connected together and fixed by bolts and nuts.
4. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 1
a cooling water path is provided in each of the covers.
5. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 3
each of the covers is shaped like a disk having a flange portion in an outer peripheral area of the cover, and the cooling water path is provided along a circumferential direction of the cover.
6. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 1
the covers are provided with a supply path and a discharge path for supplying and discharging an inert gas into and from a hollow portion of the coil.
7. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 6
each of the covers is shaped like a disk having a flange portion in an outer peripheral area of the cover, and the supply path and the discharge path for the inert gas which communicate with the hollow portion of the coil are provided in the center of the covers.
8. The apparatus for suppressing growth of an oxide film on a coil as claimed in , wherein:
claim 1
the covers are a cup for accommodating the coil and a cap for covering an opening of the cup.
9. A method for suppressing growth of an oxide film on a coil which is a spirally wound, rolled strip, comprising:
cooling the coil while covering at least opposite sides of the coil with covers.
10. The method for suppressing growth of an oxide film on a coil as claimed in , comprising:
claim 9
cooling the coil while heat insulating surfaces of the covers and the coil in intimate contact with each other.
11. The method for suppressing growth of an oxide film on a coil as claimed in , comprising:
claim 9
cooling the coil by flowing cooling water in a cooling water path provided in each of the covers.
12. The method for suppressing growth of an oxide film on a coil as claimed in , comprising:
claim 9
cooling the coil while supplying and discharging an inert gas into and from a hollow portion of the coil.
13. The method for suppressing growth of an oxide film on a coil as claimed in , comprising:
claim 9
cooling the coil in an accommodated state.