CN102200006A - 磁性纳米颗粒调剖堵水 - Google Patents
磁性纳米颗粒调剖堵水 Download PDFInfo
- Publication number
- CN102200006A CN102200006A CN2011100903495A CN201110090349A CN102200006A CN 102200006 A CN102200006 A CN 102200006A CN 2011100903495 A CN2011100903495 A CN 2011100903495A CN 201110090349 A CN201110090349 A CN 201110090349A CN 102200006 A CN102200006 A CN 102200006A
- Authority
- CN
- China
- Prior art keywords
- magnetic
- magnetic nanoparticle
- profile control
- water
- control
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明提供了一种磁性纳米颗粒调剖堵水的方法,它是将磁性纳米颗粒液体注入目的地层后,利用磁场控制磁性纳米颗粒的运动,形成牢固的纳米结构来实现的。该方法是为了能够有效地控制含水上升,而实施的磁性纳米颗粒调剖堵水。现有技术中使用的化学深部调剖堵水剂,主要进入裂缝及大孔道,对于特低渗透油藏,堵剂颗粒根本进入不了特低渗透地层孔隙,而且会污染地层。本方法所用的磁性纳米颗粒液体包括:Fe3O4磁性纳米颗粒,吐温-60,OP-21,Span-80,碳酸钠。调剖堵水时,通过对线圈电流的调控,控制磁性纳米颗粒的团聚和分散,从而实现特低渗透油藏的调剖堵水,同时可以避免化学堵水调剖剂对地层产生的污染。
Description
技术领域:
本发明涉及石油开采中调剖堵水技术。
背景技术:
堵水剂一般是指用于生产井堵水的处理剂,调剖剂则是用于注水井调整吸水剖面的处理剂。油田中采用的堵水方法分为机械堵水和化学堵水两类,化学法堵水是化学堵水剂的化学作用对出水层造成诸塞,机械法堵水是用分隔器将出水层位在井筒内卡开,以阻止水流入井内。就目前应用和发展情况看,主要是化学堵水。Fe3O4,作为一种重要的磁性材料,在磁记录、磁流体、磁性药物载体与靶向运输、医疗诊断等领域有重要而广泛的应用。当材料的尺寸减小到纳米量级时,其比表面积大大增加,且无毒,高温调剖剂的各项性能不变,将它注入地层,通过控制电源,接通电源时,实现空心线圈对磁性纳米颗粒的吸附,达到堵水的目的;当断开电源时,磁性纳米颗粒随即散开,封堵的井壁开口又开启,方便了现场应用,节能、省时省力。
发明内容:
本发明的目的就是提供一种磁性纳米颗粒调剖堵水的方法,使得磁性纳米材料注入地层后,通过控制空心线圈的电流有无,实现纳米磁性材料的团聚和分散,达到堵水的目的。
本发明的目的是这样实现的:用40℃~90℃的水与20℃~40℃的磁性纳米颗粒液体混合,磁性纳米颗粒液体为OP系列、吐温系列、Span系列等非离子表面活性剂与碳酸钠等无机盐的混合物。线圈磁感应强度为100~300Mt。地面工作站通过供电电缆控制线圈的磁场。给线圈通电,磁性纳米颗粒在磁场作用下,形成牢固的纳米结构,实现稳定封堵。断开线圈电流,磁性纳米颗粒在地层流体压力作用下,随地层流体返回地面,目的层解封。
本发明采用磁性纳米颗粒调剖堵水的概念,并开发了有效地控制磁场,使得在地面配制的水包磁性纳米颗粒液体注入地层后,在磁场作用下形成牢固的纳米颗粒结构,实现了调剖堵水的功能。同时,断开线圈电流后,磁性纳米颗粒返回地面,对地层无污染。
附图说明
图1为磁性纳米颗粒调剖堵水说明图。包括(1-供电电缆 2-磁性纳米颗粒液体泵 3-套管 4-电缆保护管 5-磁性纳米颗粒导流管 6-封隔器 7-锥形线圈固定器 8-空心锥形贴壁线圈 9-出射孔 10-封隔器 11-封隔器)
具体实施方式:
实施例一
本实施例适用地层温度为40℃~70℃工况,所用的磁性纳米颗粒液体组成:Fe3O4磁性纳米颗粒:30%,吐温-60:25%,OP-21:25%,Span-80:10%,碳酸钠:10%。
供电电缆电压:380V,线圈磁感应强度:100mT。
用温度为50℃~60℃的水70%与温度为20℃~30℃的磁性纳米颗粒液体30%混合,得到水包磁性纳米颗粒液体。对上述已生产的水包磁性纳米颗粒液体进行机械振荡,混合均匀。
将贴壁线圈用电缆放到目的地层后,用线圈固定器固定,然后将上述水包磁性纳米颗粒液体,用泵注入地下,进入地层后,对线圈加电。磁性纳米颗粒在径向磁场的作用下运行,形成牢固的纳米结构,可以稳定封堵5个月。5个月后,断开线圈电流,磁性纳米颗粒在地层流体压力作用下,随地层流体返回地面,目的层解封。
实施例二
本实施例适用地层温度为50℃~80℃工况,所用的磁性纳米颗粒液体组成:Fe3O4磁性纳米颗粒:20%,吐温-60:40%,OP-21:15%,Span-80:20%,碳酸钠:5%。
供电电缆电压:380V,线圈磁感应强度:150mT。
用温度为60℃~70℃的水50%与温度为30℃~40℃的磁性纳米颗粒液体50%混合,得到水包磁性纳米颗粒液体。对上述已生产的水包磁性纳米颗粒液体进行机械振荡,混合均匀。
将贴壁线圈用电缆放到目的地层后,用线圈固定器固定,然后将上述水包磁性纳米颗粒液体,用泵注入地下,进入地层后,对线圈加电。磁性纳米颗粒在径向磁场的作用下运行,形成牢固的纳米结构,可以稳定封堵6个月。6个月后,断开线圈电流,磁性纳米颗粒在地层流体压力作用下,随地层流体返回地面,目的层解封。
实施例三
本实施例适用地层温度为80℃~90℃工况,所用的磁性纳米颗粒液体组成:Fe3O4磁性纳米颗粒:40%,吐温-60:20%,OP-21:20%,Span-80:5%,碳酸钠:15%。
供电电缆电压:380V,线圈磁感应强度:120mT。
用温度为55℃~65℃的水45%与温度为35℃~45℃的磁性纳米颗粒液体55%混合,得到水包磁性纳米颗粒液体。对上述已生产的水包磁性纳米颗粒液体进行机械振荡,混合均匀。
将贴壁线圈用电缆放到目的地层后,用线圈固定器固定,然后将上述水包磁性纳米颗粒液体,用泵注入地下,进入地层后,对线圈加电。磁性纳米颗粒在径向磁场的作用下运行,形成牢固的纳米结构,可以稳定封堵7个月。7个月后,断开线圈电流,磁性纳米颗粒在地层流体压力作用下,随地层流体返回地面,目的层解封。
实施例四
本实施例适用地层温度为77℃~87℃工况,所用的磁性纳米颗粒液体组成:Fe3O4磁性纳米颗粒:35%,吐温-60:35%,OP-21:10%,Span-80:10%,碳酸钠:10%。
供电电缆电压:380V,线圈磁感应强度:115mT。
用温度为46℃~65℃的水45%与温度为35℃~45℃的磁性纳米颗粒液体55%混合,得到水包磁性纳米颗粒液体。对上述已生产的水包磁性纳米颗粒液体进行机械振荡,混合均匀。
将贴壁线圈用电缆放到目的地层后,用线圈固定器固定,然后将上述水包磁性纳米颗粒液体,用泵注入地下,进入地层后,对线圈加电。磁性纳米颗粒在径向磁场的作用下运行,形成牢固的纳米结构,可以稳定封堵8个月。8个月后,断开线圈电流,磁性纳米颗粒在地层流体压力作用下,随地层流体返回地面,目的层解封。
Claims (2)
1.本发明涉及一种利用磁性纳米颗粒进行调剖堵水的方法,其特征在于将磁性纳米材料注入地层后,通过控制空心线圈的电流有无,实现纳米磁性材料的团聚和分散,达到堵水的目的。磁性纳米颗粒调剖堵水的具体实施步骤如下:
步骤一.准备Fe3O4磁性纳米颗粒,按实际需要的位置,高压注入井壁地层中,纳米级的磁性颗粒作为调剖堵水剂;
步骤二.将一空心线圈,放入注磁性纳米颗粒的井壁位置,并可以随时人工控制线圈中电流的有无;
步骤三.通过控制电源,实现空心线圈对磁性纳米颗粒的吸附,磁性纳米颗粒的强吸附力,封堵井壁开口。断开电源时,磁性纳米颗粒随即散开,封堵的井壁开口又开启。
2.根据权利要求1所述的磁性纳米颗粒调剖堵水的方法,其特征是将磁性纳米颗粒注入井壁地层,通过人工控制线圈中电流的有无,实现磁性纳米颗粒的团聚和分散,从而实现调剖堵水。