CN100436611C CNB2007100986699A CN200710098669A CN100436611C CN 100436611 C CN100436611 C CN 100436611C CN B2007100986699 A CNB2007100986699 A CN B2007100986699A CN 200710098669 A CN200710098669 A CN 200710098669A CN 100436611 C CN100436611 C CN 100436611C
Authority
CN
China
Prior art keywords
cerium
hydrochloric acid
elements
control
pickling
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2007100986699A
Other languages
English (en)
Other versions
CN101033504A (zh
Inventor
徐利华
毕松梅
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University of Science and Technology Beijing USTB
Original Assignee
University of Science and Technology Beijing USTB
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University of Science and Technology Beijing USTB filed Critical University of Science and Technology Beijing USTB
Priority to CNB2007100986699A priority Critical patent/CN100436611C/zh
Publication of CN101033504A publication Critical patent/CN101033504A/zh
Application granted granted Critical
Publication of CN100436611C publication Critical patent/CN100436611C/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Images

Classifications

    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02PCLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS
    • Y02P10/00Technologies related to metal processing
    • Y02P10/20Recycling

Landscapes

  • Compounds Of Alkaline-Earth Elements, Aluminum Or Rare-Earth Metals (AREA)

Abstract

一种利用控制pH值来提纯铈的方法,属于有色冶金工业技术领域。工艺为:粉粹:将原料进行磨矿,过筛,酸洗,碱分解,盐酸优溶,过滤,沉淀。本发明的优点在于:适合低品位铈的原料。对尾矿和其他一些铈含量较低的矿物进行铈的提取,有较强的可行性;产物纯度较高,工艺操作简单,成本低,环境污染较小,对实现低品位原料的综合利用有很重要的意义。

Description

一种利用控制PH值来提纯铈的方法
技术领域
本发明属于有色冶金工业技术领域,提出了一种利用控制PH值来提纯铈的方法,并确定了最佳PH值。
背景技术
稀土在地壳中的含量为地壳重量的0.01%~0.02%,高于钨、钼、钴、铅等元素的丰度,已不是很稀少的资源了。稀土被人们誉为新世纪高科技及功能材料的宝库,它是发展高新技术的战略性元素。我国是稀土资源大国,占世界稀土储量的80%,但是我国稀土资源精矿比较少,大部分稀土堪布粒度较细,低品位稀土矿较多,因此,加强对低品位稀土矿的开采用,不仅节约了资源,实现了资源的综合利用,而且还保护环境。
目前我国所用的铈的制备方法主要有湿法和火法两种,湿法主要是通过酸碱结合,利用铈盐溶解度小的性质,最终得到铈的盐晶体;活法主要是通过氧化焙烧,硫酸浸出后直接萃取制备铈。这两种方法都适合铈品位比较高的稀土矿或者是稀土精矿。本发明所用控制PH值的方法制备铈,对低品位原料特别是白云鄂博选矿尾矿具有重要意义。
本发明工艺所用原理是根据铈的变价性和铈水解的电位一PH值图和电动势一PH值图,找出有利于铈和其他稀土分离的PH值范围。在控制溶液PH=3.0~4.0范围时,直接往溶液中加入H2O2,在Ce3+氧化成Ce4+的同时,Ge4+以Ce(OH)4的形式沉淀出来,而其他稀土元素的水解都在PH>6.0之后,这样就实现了铈与其它元素的初步分离。
虽然目前国内在在资源利用技术领域中有关湿法和火法提取铈的已有专利申请,但在以尾矿和含铈低品位矿物为对象的环境技术领域利用控制PH值的方法提取铈的专利还没有。因此本发明在含铈品位较低的冶炼中,是一项新的工艺。
发明内容
本发明的目的在于提供一种利用控制PH值来提纯铈的方法,一是对尾矿进行有价元素的回收,实现资源的综合利用;二是提取一种适合玻璃陶瓷和钢铁冶金所用原料的廉价制备方法,降低原料成本。
本发明的工艺步骤如下:
(1)粉粹:将原料进行磨矿,过0.074mm筛。
(2)酸洗:用浓盐酸搅拌酸洗6-8小时,除铁、钙和硅。
(3)碱分解:用60-85%的NaOH在130-150℃反应1-1.5小时,目的在于使氟碳铈矿分解为稀土氢氧化物。
(4)盐酸优溶:根据各元素的溶解度不同,实现易溶元素与难溶元素的分离。控制PH=1.0-1.5,使稀土元素和其他可溶性离子进入溶液中,并加入H2O2,还原四价铈为三价,以促进Ce(OH)4的充分溶解。
(5)过滤:先用一层滤纸进行过滤,滤液再用两层滤纸过滤,以更能有效的去处微细沉淀杂质。
(6)沉淀:控制滤液PH=3.0-4.0,并同时加入适量的H2O2,直到溶液颜色不再发生变化为止,使铈以Ce(OH)4的形式沉淀出来,实现了与其他元素的分离。
本发明的优点在于:
(1)适合低品位铈的原料。对尾矿和其他一些铈含量较低的矿物进行铈的提取,有较强的可行性。
(2)工艺操作简单,成本低,减少了对环境的污染。
附图说明
图1是通过控制不同的PH值所做对比试验图。
图2是实例1所做试验结果。
图3是实例2所做试验结果。
具体实施方式
以下通过对实施例的描述来介绍本发明的具体实施方式。
实例1:
将白云鄂博选矿尾矿粉粹至粒径小于0.074mm,取出经粉碎的矿石50g,用浓盐酸酸洗7小时之后,滤出不溶物,用70%的NaOH在140℃反应40min,再进行盐酸优溶,用NaOH对优溶液进行滴定,控制PH=4.0,所得沉淀中铈的纯度为16.32%。
实例2:
将白云鄂博选矿尾矿粉粹至粒径小于0.074mm,取出经粉碎的矿石25g,用浓盐酸酸洗7小时之后,滤出不溶物,用70%的NaOH在140℃反应40min,再进行盐酸优溶,用NaOH对优溶液进行滴定,控制PH=3.5,所得沉淀中铈的纯度为20.38%。

Claims (1)

1、一种利用控制PH值来提纯铈的方法,其特征在于:工艺步骤为:
a、粉粹:将原料进行磨矿,过0.074mm筛;
b、酸洗:用浓盐酸搅拌酸洗6-8小时,除铁、钙和硅;
c、碱分解:用60-85%的NaOH在130-150℃反应1-1.5小时,使氟碳铈矿分解为稀土氢氧化物;
d、盐酸优溶:根据各元素在酸溶液中的溶解度不同,实现易溶元素与难溶元素的分离;控制PH=1.0-1.5,使稀土元素和其他可溶性离子进入溶液中,并加入H2O2,还原四价铈为三价,以实现在优溶过程中所产生的Ce(OH)4溶解;
e、过滤:先用一层滤纸进行过滤,滤液再用两层滤纸过滤,去除微细沉淀杂质;
f、沉淀:控制上述滤液PH=3.0-4.0,并同时加入H2O2,直到溶液颜色不再发生变化为止,使铈元素以Ce(OH)4的形式沉淀出来,实现了与其他元素的分离。
CNB2007100986699A 2007-04-24 2007-04-24 一种利用控制ph值来提纯铈的方法 Expired - Fee Related CN100436611C (zh)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CNB2007100986699A CN100436611C (zh) 2007-04-24 2007-04-24 一种利用控制ph值来提纯铈的方法

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CNB2007100986699A CN100436611C (zh) 2007-04-24 2007-04-24 一种利用控制ph值来提纯铈的方法

Publications (2)

Publication Number Publication Date
CN101033504A CN101033504A (zh) 2007-09-12
CN100436611C true CN100436611C (zh) 2008-11-26

Family

ID=38730245

Family Applications (1)

Application Number Title Priority Date Filing Date
CNB2007100986699A Expired - Fee Related CN100436611C (zh) 2007-04-24 2007-04-24 一种利用控制ph值来提纯铈的方法

Country Status (1)

Country Link
CN (1) CN100436611C (zh)

Families Citing this family (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101649393B (zh) * 2008-08-12 2011-05-11 兰州大学 从含轻金属的混合溶液中富集低浓度有价金属的方法
CN101824554B (zh) * 2010-03-12 2013-06-12 瑞科稀土冶金及功能材料国家工程研究中心有限公司 一种混合稀土精矿液碱焙烧分解提取工艺
CN104388711A (zh) * 2014-12-11 2015-03-04 内蒙古科技大学 稀土氧化物熔渣浸出回收稀土方法
CN111996396A (zh) * 2020-08-26 2020-11-27 江西理工大学 一种稀土料液除铈及非稀土杂质的方法

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1994023075A1 (en) * 1990-09-19 1994-10-13 Union Oil Company Of California Recovery of cerium from fluoride-containing ores
CN1236017A (zh) * 1999-06-25 1999-11-24 清华大学 氯化铵法从氟碳铈精矿提取氯化稀土的方法

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1994023075A1 (en) * 1990-09-19 1994-10-13 Union Oil Company Of California Recovery of cerium from fluoride-containing ores
CN1236017A (zh) * 1999-06-25 1999-11-24 清华大学 氯化铵法从氟碳铈精矿提取氯化稀土的方法

Also Published As

Publication number Publication date
CN101033504A (zh) 2007-09-12

Similar Documents

Publication Publication Date Title
CN106191477B (zh) 从海底钴锰多金属氧化矿中分离回收稀土的方法
CN105331837B (zh) 一种从赤泥中富集钪的方法
CN103555938A (zh) 一种高含泥氧化铜矿的选冶方法
CN102329955A (zh) 全湿法处理红土镍矿生产电解镍的综合方法
CN101831542B (zh) 一种从钼选矿尾矿中提取金属元素铁、镁、钙的方法
CN106367590A (zh) 一种独居石矿综合利用回收工艺
CN103526019B (zh) 一种从多金属伴生钒矿中综合回收钒硒银的方法
CN114752774A (zh) 一种赤泥中铁铝分离的方法
CN100436611C (zh) 一种利用控制ph值来提纯铈的方法
CN105349792B (zh) 一种黄铜炉渣回收再利用工艺
CN104962739A (zh) 一种风化壳淋积型稀土矿稀土浸出液的快速除杂方法
CN104480316A (zh) 一种从钕铁硼磁材废料中回收Co元素的简便化工业方法
CN110205493A (zh) 钴渣与镍钼矿混合浸出提取钴、镍的方法
CN1861817A (zh) 从磁铁矿尾渣中提取金属钴的工艺
CN103952533B (zh) 利用煅烧、碱浸及脱泥再选钒钛磁铁精矿的方法
CN100500570C (zh) 一种从选铁尾矿中制备二氧化铈的方法
CN103977880B (zh) 利用碱浸、脱泥及磁重联合再选钒钛磁铁精矿的方法
CN111411224B (zh) 一种从低品位含锰矿石中综合回收结合银铜的选矿方法
CN105110300A (zh) 一种含硫化锰的复合锰矿提取锰及硫的方法
CN103962222B (zh) 利用煅烧、碱浸、脱泥及磁选再选钒钛磁铁精矿的方法
CN102732720B (zh) 一种处理氧化铜矿的方法
CN104263926A (zh) 含钪超基性岩的提钪工艺
CN105543494A (zh) 一种冶选联合分步回收渣中有价金属的方法
CN104975192A (zh) 从含钪物料中提取钪的方法
CN116287705A (zh) 一种草酸浸出含铌粗精矿中铌、钛、铁的方法

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
C14 Grant of patent or utility model
GR01 Patent grant
C17 Cessation of patent right
CF01 Termination of patent right due to non-payment of annual fee

Granted publication date: 20081126

Termination date: 20110424