CN104774505A - New material for painting material of oil wax painting - Google Patents
New material for painting material of oil wax painting Download PDFInfo
- Publication number
- CN104774505A CN104774505A CN201410015138.9A CN201410015138A CN104774505A CN 104774505 A CN104774505 A CN 104774505A CN 201410015138 A CN201410015138 A CN 201410015138A CN 104774505 A CN104774505 A CN 104774505A
- Authority
- CN
- China
- Prior art keywords
- wax
- painting
- prepared
- oily
- blended wax
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a new material for a painting material of an oil wax painting, wherein the new material comprises the raw materials: 0.25 wt% of an environmentally friendly paint, 10.00-15.00 wt% of white oil, 3.00-5.00 wt% of hardened oil, 4.00-4.05 wt% of paraffin, 3.50-4.50 wt% of chewing gum wax, 20.00-24.00 wt% of mixed wax, 50.00-58.00 wt% of nano calcium carbonate, and 0-0.20 wt% of medical vaseline, wherein the mixed wax is prepared by mixing 95.00 wt% of stearic acid and 5.00 wt% of magnesium oxide. According to the formula and the production method thereof, the painting material which is environmentally friendly, non-toxic and beautiful in colors, can be easy to color and is not easy to rupture and long in shelf life can be prepared.
Description
Technical field
The present invention relates to a kind of drawing instrument material, particularly a kind of oily encaustic painting draws formula of material and preparation method thereof.
Background technology
Modal graphic products mainly artistic oil painting stick and wax crayon, although this series products can meet general drawing requirement, also has its weak point in the market.
Wax crayon exists that colouring is uneven, and color is bright and beautiful not, and available drawing means are more single, and it is not ideal enough to draw performance, is in particular in repeat when painting is retouched even not, and level of coverage is inadequate, and the quality guaranteed period of wax crayon is shorter, and flexural capacity is poor, easy fracture.
Comparatively speaking, artistic oil painting stick feel is fine and smooth, smooth, spreadability is good, folded look, colour mixture excellent performance, but its pattern color drawn out is more flat and bright-coloured not bright and beautiful.In addition, containing a certain amount of soluble heavy metal element in the raw material of artistic oil painting stick, they are brought into by raw pigment often, as lead, barium, chromium, antimony, cadmium, mercury, arsenic etc., take in these heavy metal elements unawares, harm can be produced to human body to a certain extent.Have data to show, in the Toy Safety Standards of China, for the pigment of children, the prohibitive content of the heavy metal elements such as lead, barium, chromium, antimony, cadmium, mercury, arsenic and compound thereof, compared with the Toy Safety Standards of the European Community, seems that some requires too low.So growing up healthy and sound in order to child, painting material and the apparatus of exploitation safety and environmental protection are very necessary.
Summary of the invention
For solving the deficiencies in the prior art, the invention provides a kind of environment-protecting asepsis, bright in colour bright and beautiful, drawing excellent property, and the stronger oily encaustic painting of fracture resistence force draws formula of material and preparation method thereof.
The technical solution used in the present invention is: a kind of oily encaustic painting draws material novel material, it is prepared from by following composition of raw materials: environmental-friendly pigment 0.25wt%, white oil 10.00 ~ 15.00wt%, winterized stearin 3.00 ~ 5.00wt%, paraffin 4.00 ~ 4.05wt%, chewing gum wax 3.50 ~ 4.50wt%, blended wax 20.00 ~ 24.00wt%, nano-calcium carbonate 50.00 ~ 58.00 wt%, medical ventolin 0 ~ 0.20wt%; Described blended wax is prepared from by following material: stearic acid, magnesium oxide.
Further, preferred composition of raw materials ratio is each raw material weight per-cent: environmental-friendly pigment 0.25wt%, white oil 12.00 ~ 14.19wt%, winterized stearin 4.00 ~ 4.05wt%, paraffin 4.00 ~ 4.05wt%, chewing gum wax 4.00 ~ 4.05wt%, blended wax 22.50 ~ 22.78wt%, nano-calcium carbonate 50.63 ~ 53.00wt%, medical ventolin 0 ~ 0.20wt%; Described blended wax is prepared from by following material: stearic acid, magnesium oxide.
Prepare the method that oily encaustic painting draws material novel material, comprise the steps:
1.. the raw material of corresponding weight percent is taken according to above-mentioned formula rate, stand-by;
2.. in Scattered Kettle, add white oil, winterized stearin, environmental-friendly pigment, stirring at low speed and high speed dispersion synchronously carry out 30mins;
3. the mixture in Scattered Kettle is placed in grinding machine for grinding, is rolled into required process colour, material is irregular solid state;
4. by step 3. in irregular solid state material be placed in and dissolve cylinder and heat, temperature is set to 100 oC ± 2 oC, drops into paraffin, chewing gum wax, blended wax, nano-calcium carbonate, medical ventolin, Heat preservation for some time, dissolves into liquid;
5. liquid is poured into stirrer, low speed uniform stirring 40mins ~ 50mins;
6. by the mould of liquid injection molding machine, condensation is shaping.
Wherein, the preparation process of described blended wax is: add stearic acid 10.00wt%, magnesium oxide 5.00wt% in a kettle., and temperature controls at 210oC ± 2 oC, low speed uniform stirring 30mins, then add the stearic acid of 85.00 wt%, after fully dissolving, stop insulation, after cooling, make blended wax.
Oily encaustic painting of the present invention is drawn material novel material and is referred to a kind of new formula materials for making the bar-shaped paintbrush of oily encaustic painting; The present invention's winterized stearin used, chewing gum wax, environmental-friendly pigment are commercially available, and wherein the buying of chewing gum wax is from Nanyang wax Fine Chemical Works, can also replace with other commercially available chewing gum wax.For environmental-friendly pigment, there is no particular restriction for its color, as long as can not produce detrimentally affect to object of the present invention, those skilled in the art easily can draw material according to required oily encaustic painting and select suitable environmental-friendly pigment.As black series pigments can such as but be not limited only to be carbon black; Same, the pigment of red colour system, blue series, green system, yellow system can be one or more, not specific single restriction, as long as rear and required consistent of allotment.
After oil encaustic painting draws material fabrication of new materials, through a QC acceptance certificate weight at 8g ± 0.3g, production specification is 7.5 × 1.2cm is qualified product, winder wraps up in mark, Processing Criterion mounted box, vanning on request, environmental protection, nontoxic, beautiful in colour, coloring solution, the not painting material of easy fracture, long quality-guarantee period can be processed into.
Oily encaustic painting of the present invention is drawn material novel material tool and is had the following advantages:
(1) environment-protecting asepsis, tasteless; Adopt environmental-friendly pigment to replace the original pigment used, the substances content that heavy metal etc. is detrimental to health is far below international limit standard;
(2) feel is fine and smooth, smooth, spreadability is good, folded color contamination look excellent performance, and color is vivid, and drawing layer thickens, coating is ultra-fine, and more have texture, coating wt reaches 198g/m
2;
(3) long quality-guarantee period, can persistence in the shady and cool dry ventilation, indoor lower than 50 oC;
(4) close structure, resistance to fracture is strong, not frangibility and loss;
(5) formula environmental protection, production process is to human body, environmental nonpollution, and the recyclable re-using of scrap stock in production process, recycle is worth high, and economical effectiveness is obvious.
Embodiment
Embodiment 1
The formula of raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 10.00 ~ 15.00wt%, winterized stearin 3.00 ~ 5.00wt%, paraffin 4.00 ~ 4.05wt%, chewing gum wax 3.50 ~ 4.50wt%, blended wax 20.00 ~ 24.00wt%, nano-calcium carbonate 50.00 ~ 58.00 wt%, medical ventolin 0 ~ 0.20wt%.
First blended wax is prepared: add stearic acid 10.00wt%, magnesium oxide 5 .00wt% in a kettle., temperature controls at 210oC ± 2oC, low speed uniform stirring 30mins, add the stearic acid of 85.00 wt% again, after abundant dissolving, stop insulation, after cooling, make blended wax.
Then, in Scattered Kettle, add white oil, winterized stearin, environmental-friendly pigment, stirring at low speed and high speed dispersion synchronously carry out 30mins; Then mixture is placed in grinding machine for grinding, is rolled into the irregular solid state of required process colour; Gone to dissolve in cylinder by material again and heat, temperature is arranged on 100 oC ± 2 oC, drops into paraffin, chewing gum wax, blended wax, nano-calcium carbonate, medical ventolin, Heat preservation for some time, dissolves into liquid; Then, liquid pours stirrer into, low speed uniform stirring 40mins ~ 50mins; Finally by liquid injection molding machine mould, condensation is shaping, is oily encaustic painting and draws material novel material.
QC acceptance certificate Zhi Zhiliang is 8g ± 0.3g, and production specification is 7.5 × 1.2cm, and winder wraps up in mark, by package processing standard mounted box, vanning, novel environment friendly, nontoxic, beautiful in colour, painted easily, the painting material of not easy fracture.
Embodiment 2
The formula of raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 12.00wt%, winterized stearin 4.50wt%, paraffin 4.00wt%, chewing gum wax 4.00wt%, blended wax 24.00wt%, nano-calcium carbonate 51.25 wt%.
First blended wax is prepared: add stearic acid 10.00wt%, magnesium oxide 5.00 wt% in a kettle., temperature controls at 210oC ± 2 oC, low speed uniform stirring 30mins, add the stearic acid of 85.00 wt% again, after abundant dissolving, stop insulation, after cooling, make blended wax.
Then, in Scattered Kettle, add white oil, winterized stearin, environmental-friendly pigment, stirring at low speed and high speed dispersion synchronously carry out 30mins; Then mixture is placed in grinding machine for grinding, is rolled into the irregular solid state of required process colour; Gone to dissolve in cylinder by material again and heat, temperature is arranged on 100 oC ± 2 oC, drops into paraffin, chewing gum wax, blended wax, nano-calcium carbonate, medical ventolin, Heat preservation for some time, dissolves into liquid; Then, liquid pours stirrer into, low speed uniform stirring 45mins; Finally by liquid injection molding machine mould, condensation is shaping, is oily encaustic painting and draws material novel material.
QC acceptance certificate Zhi Zhiliang is 8g ± 0.3g, and production specification is 7.5 × 1.2cm, and winder wraps up in mark, by package processing standard mounted box, vanning, novel environment friendly, nontoxic, beautiful in colour, painted easily, the painting material of not easy fracture, long quality-guarantee period.
Embodiment 3
The formula of raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.19wt%, winterized stearin 4.05wt%, paraffin 4.05wt%, chewing gum wax 4.05wt%, blended wax 22.78wt%, nano-calcium carbonate 50.43 wt%, medical ventolin 0.20wt%.
First blended wax is prepared: add stearic acid 10.00wt%, magnesium oxide 5.00 wt% in a kettle., temperature controls at 210oC ± 2 oC, low speed uniform stirring 30mins, add the stearic acid of 85.00 wt% again, after abundant dissolving, stop insulation, after cooling, make blended wax.
Then, in Scattered Kettle, add white oil, winterized stearin, environmental-friendly pigment, stirring at low speed and high speed dispersion synchronously carry out 30mins; Then mixture is placed in grinding machine for grinding, is rolled into the irregular solid state of required process colour; Gone to dissolve in cylinder by material again and heat, temperature is arranged on 100 oC ± 2 oC, drops into paraffin, chewing gum wax, blended wax, nano-calcium carbonate, medical ventolin, Heat preservation for some time, dissolves into liquid; Then, liquid pours stirrer into, low speed uniform stirring 40mins; Finally by liquid injection molding machine mould, condensation is shaping, is oily encaustic painting and draws material novel material.
QC acceptance certificate Zhi Zhiliang is 8g ± 0.3g, and production specification is 7.5 × 1.2cm, and winder wraps up in mark, by package processing standard mounted box, vanning, novel environment friendly, nontoxic, beautiful in colour, long quality-guarantee period painting material.It is easily painted that the oily encaustic painting that this embodiment makes draws material novel material, and drawing performance is at 198g/m
2; Anti-breaking force is 6N, not easy fracture.
Embodiment 4
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.00wt%, winterized stearin 4.20wt%, paraffin 4.00wt%, chewing gum wax 4.20wt%, blended wax 22.50wt%, nano-calcium carbonate 50.65wt%, medical ventolin 0.20wt%.
Embodiment 5
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.10wt%, winterized stearin 3.90wt%, paraffin 4.05wt%, chewing gum wax 4.05wt%, blended wax 23.00wt%, nano-calcium carbonate 50.45wt%, medical ventolin 0.20wt%.
Embodiment 6
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 13.50wt%, winterized stearin 4.10wt%, paraffin 4.05wt%, chewing gum wax 3.90wt%, blended wax 22.80wt%, nano-calcium carbonate 51.30wt%, medical ventolin 0.10wt%.
Embodiment 7
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.20wt%, winterized stearin 3.65wt%, paraffin 4.03wt%, chewing gum wax 3.95wt%, blended wax 23.50wt%, nano-calcium carbonate 50.22wt%, medical ventolin 0.20wt%.
Embodiment 8
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 13.98wt%, winterized stearin 3.85wt%, paraffin 4.04wt%, chewing gum wax 4.15wt%, blended wax 22.60wt%, nano-calcium carbonate 50.98wt%, medical ventolin 0.15wt%.
Embodiment 9
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.50wt%, winterized stearin 4.05wt%, paraffin 4.05wt%, chewing gum wax 4.05wt%, blended wax 22.78wt%, nano-calcium carbonate 50.12wt%, medical ventolin 0.20wt%.
Embodiment 10
Make oily encaustic painting by the step described in embodiment 3 and draw material novel material, formula unlike raw material is as follows: environmental-friendly pigment 0.25wt%, white oil 14.19wt%, winterized stearin 4.15wt%, paraffin 4.05wt%, chewing gum wax 4.05wt%, blended wax 21.95wt%, nano-calcium carbonate 51.16wt%, medical ventolin 0.20wt%.
Claims (4)
1. an oily encaustic painting draws material novel material, it is characterized in that: be prepared from by following composition of raw materials: environmental-friendly pigment 0.25wt%, white oil 10.00 ~ 15.00wt%, winterized stearin 3.00 ~ 5.00wt%, paraffin 4.00 ~ 4.05wt%, chewing gum wax 3.50 ~ 4.50wt%, blended wax 20.00 ~ 24.00wt%, nano-calcium carbonate 50.00 ~ 58.00 wt%, medical ventolin 0 ~ 0.20wt%; Described blended wax is prepared from by following material: 95.00 wt% stearic acid, 5.00 wt% magnesium oxide.
2. oily encaustic painting according to claim 1 draws material novel material, it is characterized in that: it is prepared from by following composition of raw materials: environmental-friendly pigment 0.25wt%, white oil 12.00 ~ 14.19wt%, winterized stearin 3.50 ~ 4.50wt%, paraffin 4.00 ~ 4.05wt%, chewing gum wax 4.00 ~ 4.05wt%, blended wax 22.50 ~ 22.78wt%, nano-calcium carbonate 50.63 ~ 53.00 wt%, medical ventolin 0 ~ 0.20wt%; Described blended wax is prepared from by following material: 95.00 wt% stearic acid, 5.00 wt% magnesium oxide.
3. the oily encaustic painting prepared described in claim 1 or 2 draws the method for material novel material, it is characterized in that: comprise the steps:
1.. the composition of raw materials of corresponding weight percent is taken according to claim 1 or 2, stand-by;
2.. in Scattered Kettle, add white oil, winterized stearin, environmental-friendly pigment, stirring at low speed and high speed dispersion synchronously carry out 30mins;
3. the mixture in Scattered Kettle is placed in grinding machine for grinding, is rolled into required process colour, material is irregular solid state;
4. by step 3. in irregular solid state material be placed in and dissolve cylinder and heat, temperature is set to 100 oC ± 2 oC, drops into paraffin, chewing gum wax, blended wax, nano-calcium carbonate, medical ventolin, Heat preservation for some time, dissolves into liquid;
5. liquid is poured into stirrer, low speed uniform stirring 40mins ~ 50mins;
6. by the mould of liquid injection molding machine, condensation is shaping.
4. the oily encaustic painting as described in as arbitrary in claim 1-3 draws material novel material, it is characterized in that: the preparation process of described blended wax is: add stearic acid 10.00wt%, magnesium oxide 5.00wt% in a kettle., temperature controls at 210oC ± 2 oC, low speed uniform stirring 30mins, add the stearic acid of 85.00 wt% again, after abundant dissolving, stop insulation, after cooling, make blended wax.